Wednesday, February 4, 2009

Kneading with the Big Kneader

Since the cleaning of the big kneader takes about at least two hours the kneading was started early in the morning. Now it is with the same Arg. body and 8mm fibers and same as earlier the test samples had to be taken out at intervals. After 4 hours and 45 minutes, we tried to vacuum the device to make an extrusion of the kneaded material but the vacuuming seemed to be not working. Hence, the extrusion was stopped and cleaning started, it took about 3 hours to be finished.

For another project I had to give hand by doing a test on three samples. Each and every sample had to be placed in hot water of which the temperature had to be between 500 - 600 degrees. The beaker with water was placed on the electronic heater (electronic hotplate) and when the temperature was in equilibrium in between the mentioned temperature a sample (Tablet like) was carefully put into the middle using a tweezers. After five hours the samples had to be taken out and dried and weigh. The intention was to remove the binder which is dissoluble in water.
The weight of the first sample has reduced but it was kept to be dried more in air.

Tuesday, February 3, 2009

Kneading with Glass Fibers (small kneader)

Kneading of the Arg. body was started in the morning with glass fibers using the small kneader and it had to be kneaded for five hours and test samples had to be taken out after 30min and each and every hour. These samples will be sieved and fibers will be separated to observe the length of the kneaded glass fibers. Cleaning of this small kneader takes about 45 min to one hour.
The kneading has to be done using the big kneader so that it was cleaned off the oil and fixed for the next day use.
Al2O3 fibers still break up in the sintering process even this time another program was used. Now I am going to check whether the heating rate at the beginning has something to do with the fiber explosion.

Monday, February 2, 2009

Failure in the Sintering Process

As a sample of test sample 2 was put to the furnace CeramAix to sinter I looked at the results today in the morning. But there was no sample left on the Zirconia substrate. Probably the fiber is broken into pieces and blown away with the heat flow.

Since it is arguable about the inside flows which can break the structure of the fibers, the use of a crucible would be a good idea and I was provided with a crucible. Using it another sample was put to the furnace and this time it will go upto 14000C and sinter Al2O3.

Friday, January 30, 2009

Al2O3 Program Change

Since there was no change of the result of firing Al2O3 fibers with slower heating rates we (with the supervisor) decided to use a higher rate and check the results.
Using the changed program I put a sample to the furnace.

Kneading of another sample of bare body was done for 5 hours with the EMU Memo which logs the current used during kneading within every one minute period. Cleaning of the machine took about 30 mins.

As today is Friday lab cleaning was done at 2 O' clock.

Thursday, January 29, 2009

Al2O3 Second Firing Results

Al2O3 sintered fibers were taken out from the kiln. But as the problem occurred in the previous firing, after this firing there was no fibers found. Everything is broken into pieces. Have to find a solution for this problem.

Wednesday, January 28, 2009

Kneading Material

For the project Arg, another sample of body should be kneaded with fibers inside 6%. Hence, the kneading was started but after some time it was observed that the kneaded was stopped. There was a problem with the power outlet so that the kneading had to be started from the scratch.

Compression test for the third batch of project MH was done. It showed some interesting results. According to that clay with different kinds of silica had different strengths. According to strength,
1. Double layer Silica
2. Single layer Silica
3. Mixed Silica (Double and Single layer)

Tuesday, January 27, 2009

Sample Preparation

In the morning had a meeting with the co-supervisor and granted some work that has to be done within next few days. For one project (Arg) I have to do 3 kneadings.

1. with fibers - 6% - 5 hrs
2. with glass fibers - 6% - 5hrs
3. without fibers - 5 hrs

and also prepare samples for compression test on project MH and help my colleague for that.

So started work with kneading the sample without fibers.
Then sample preparation of MH for the compression test.

In the evening started to clean the small kneader after getting instructions from the co-supervisor.